Home » News » Industry News » What Is Duplex 2205 Stainless Steel?

What Is Duplex 2205 Stainless Steel?

Views: 9     Author: Monica     Publish Time: 2026-10-16      Origin: Site

twitter sharing button
wechat sharing button
whatsapp sharing button
linkedin sharing button
pinterest sharing button
facebook sharing button
sharethis sharing button

What Is Duplex 2205 Stainless Steel?

Duplex 2205 is a dual-phase stainless steel whose annealed structure is about 50 percent ferrite and 50 percent austenite. That two-phase mix gives it roughly twice the yield strength of 316L together with chloride pitting and stress-corrosion resistance that 316L cannot match. Its primary designation is UNS S32205, with EN 1.4462 the European equivalent and F60 the forged grade code.

What Is Duplex 2205 Stainless Steel.webp

Duplex 2205 belongs to the family of duplex (austenitic-ferritic) stainless steels. The word "duplex" describes the microstructure: instead of the fully austenitic grains of 304 or 316, the material contains two interlocked crystal phases. Each phase contributes different strengths - the ferrite supplies strength and resistance to chloride stress-corrosion cracking, while the austenite supplies toughness, ductility and corrosion resistance. The result is a grade that is stronger than austenitic stainless yet tougher and more weldable than ferritic stainless.

The grade was developed in the early 1980s as the second-generation duplex, improving on the first commercial duplex (UNS S31803) by tightening the chromium range and raising nitrogen. Today UNS S32205 is the active grade most specifications call for, while the older S31803 remains valid and is still produced. If you want the naming background, see how the duplex numbering system works and what UNS S31803 is.

  • Microstructure: roughly 50 percent ferrite + 50 percent austenite after solution annealing.

  • Primary grade: UNS S32205 (older UNS S31803 still in use).

  • European grade: EN 1.4462 (Werkstoff 1.4462).

  • Forged grade code: F60 (S32205) and F51 (S31803).

  • Place in the family: sits between 316L and Super Duplex 2507 in strength and corrosion resistance.

Why Is It Called Duplex, and What Does 2205 Mean?

"Duplex" means the metal carries two crystal phases - ferrite and austenite - in roughly equal amounts. The "2205" name comes from the original nominal 22 percent chromium and 5 percent nickel balance that defined the grade, even though modern S32205 tolerances are tighter than that early recipe.

Stainless steels are usually named by their dominant phase: ferritic grades (430) are mostly ferrite, austenitic grades (304, 316) are fully austenite. Duplex deliberately keeps both. The ferrite gives high strength and resistance to chloride stress-corrosion cracking; the austenite gives the ductility and toughness needed for forming and impact loading.

The numeric label is historical marketing shorthand. The first successful commercial duplex was designed around 22 percent chromium and 5 percent nickel - hence "2205". Modern UNS S32205 keeps the spirit but tightens it: chromium becomes 22.0-23.0 percent and nitrogen is raised to 0.14-0.20 percent to lock in the phase balance and strength. So the name is a family label, not a precise composition statement. Our duplex vs super duplex overview explains where 2205 sits relative to 2507.

What Is the Chemical Composition of Duplex 2205?

The active grade is UNS S32205: 22.0-23.0 percent chromium, 4.5-6.5 percent nickel, 3.0-3.5 percent molybdenum, 0.14-0.20 percent nitrogen, with carbon at or below 0.030 percent. The nitrogen is the key modern addition - it lets the grade reach high strength and a high PREN while still holding the ferrite-austenite balance.

What Is the Chemical Composition of Duplex 2205.webp

Composition is controlled tightly because the balance of phases depends on it. Too little chromium or nitrogen shifts the structure toward austenite and loses the strength advantage; too much ferrite-former can push the structure ferritic and hurt toughness. The table below compares the two duplex designations you will meet on certificates.

Duplex 2205 chemical composition (ladle analysis, weight percent)

Element

UNS S31803

UNS S32205

Carbon, max

0.030

0.030

Chromium

21.0-23.0

22.0-23.0

Nickel

4.5-6.5

4.5-6.5

Molybdenum

2.5-3.5

3.0-3.5

Nitrogen

0.08-0.20

0.14-0.20

Manganese, max

2.00

2.00

Silicon, max

1.00

1.00

Phosphorus, max

0.030

0.030

Sulfur, max

0.020

0.020

Iron

Balance

Balance

For procurement, specify UNS S32205 rather than S31803: the higher and tighter nitrogen gives more consistent corrosion resistance and strength. You can review the pipe-specific chemistry and tolerances in our ASTM A790 S31803/S32205 pipe page.

How Does Duplex 2205 Resist Corrosion, and What Is Its PREN?

2205 resists chloride pitting and chloride stress-corrosion cracking far better than 316L because its PREN of 34-38 pushes the pitting potential above typical service temperatures. It is not immune in hot concentrated chloride, however - that is exactly the condition where Super Duplex 2507 (UNS S32750) takes over.

PREN (Pitting Resistance Equivalent Number) is calculated as %Cr + 3.3 x %Mo + 16 x %N. For 2205 the chromium, molybdenum and especially nitrogen combine to a PREN of about 34-38. By contrast, 316L lands near 24-26. The higher PREN raises the temperature at which pitting starts, so 2205 survives seawater splash, desalination and process chloride that would pit 316L.

PREN and chloride performance across common grades

Grade

Typical PREN

Chloride pitting (CPT, ~)

Chloride SCC resistance

316L

24-26

Low (pitters early in chloride)

Poor

904L

32-36

Moderate

Fair

Duplex 2205

34-38

Good

Excellent

Super Duplex 2507 (S32750)

38-42

Very high

Superior

Rule of thumb: 2205 is the right call when chlorides, strength and cost together rule out 316L, but step up to Super Duplex S32750 once chloride exceeds about 10,000 ppm or seawater temperature rises above roughly 35 C.

How Does Duplex 2205 Compare with 316L Stainless Steel?

2205 delivers about 2.6 times the yield strength of 316L (450 MPa vs 170 MPa) and a PREN roughly 10 points higher, at a moderate cost premium. The trade-off is more fabrication sensitivity: 2205 must be kept out of the 280-520 C range and welded with controlled interpass temperature.

The practical consequence of the strength gap is wall thickness. For the same pressure and diameter, a 2205 pipe can be 30-50 percent thinner than a 316L pipe, which offsets the higher alloy price on a finished-component basis. That is why 2205 dominates offshore topsides and seawater systems where weight and chloride both matter.

Duplex 2205 vs 316L at a glance

Property

316L (S31603)

Duplex 2205 (S32205)

Implication

Yield strength, min

170 MPa (25 ksi)

450 MPa (65 ksi)

Thinner walls with 2205

Tensile strength, min

485 MPa (70 ksi)

620-655 MPa (90-95 ksi)

Higher pressure rating

Elongation, min

40%

25%

316L more formable

PREN

24-26

34-38

2205 far better in chloride

Chloride SCC

Poor

Excellent

Key reason to upgrade

Max continuous temp

~870 C oxidation

~300 C (phase limits)

316L for high heat

Relative cost

Low

Medium

2205 premium on material only

If your question is simply "316L or 2205?", start with the environment comparison of 2205 against 2507 to set the upper bound, then confirm against 316L using the table above.

What Are the Mechanical Properties of Duplex 2205?

Solution-annealed 2205 delivers a minimum yield of 450 MPa (65 ksi) and tensile of 620-655 MPa (90-95 ksi) with at least 25 percent elongation and hardness capped near 290 HBW. That is about 2.6 times the yield of 316L at comparable ductility, which is the single most useful design property of the grade.

What Are the Mechanical Properties of Duplex 2205.webp

Typical mechanical properties, solution-annealed (ASTM A789/A790/A240)

Property

UNS S31803

UNS S32205

Test basis

Tensile strength, min

620 MPa (90 ksi)

655 MPa (95 ksi)

Room temperature

Yield strength (0.2%), min

450 MPa (65 ksi)

450 MPa (65 ksi)

Room temperature

Elongation, min

25%

25%

50 mm gauge

Hardness, max

290 HBW / 31 HRC

290 HBW / 31 HRC

As-annealed

Charpy impact, min

~27 J at -46 C

~27 J at -46 C

Low-temperature toughness

Note that ASTM A790 lists S31803 at 620 MPa tensile and S32205 at 655 MPa; many mills report typical values well above the minima (yield often 500-580 MPa). Design with the minimum, buy against the certificate. For pressure equipment, read the allowable stress from ASME Section II Part D at your design temperature rather than from the tabulated minimum.

What Is the Dual-Phase Microstructure and Ferrite Balance Requirement?

The useful properties of 2205 depend on holding 40-60 percent ferrite (mills normally target 45-55 percent). Too much ferrite loses toughness and corrosion resistance; too little forfeits the strength and chloride-SCC advantage over austenitic stainless. Ferrite is measured by ferritescope or ASTM E562 and reported on the material certificate.

Because the two phases form and grow during cooling from the solution-annealing temperature, the balance is sensitive to chemistry, annealing temperature and quench rate. A heat that ends up at 70 percent ferrite will be hard and brittle; one at 30 percent ferrite behaves almost like 316L and loses the duplex benefit. That is why ferrite measurement is a mandatory quality control step, not an optional extra.

Effect of ferrite content on 2205 behaviour

Ferrite fraction

Consequence

Action

< 35-40%

Approaches austenitic behaviour; loses SCC strength edge

Reject or re-anneal

40-60% (target 45-55%)

Full duplex benefit: strength + toughness + SCC resistance

Accept

> 65%

Lower toughness, higher sensitization risk

Reject or re-anneal

What Are the Physical Properties of Duplex 2205?

2205 has a density of 7.8 g/cm3, an elastic modulus of 200 GPa, thermal expansion close to carbon steel, and thermal conductivity roughly three times that of 316L. Because of its ferrite content it is ferromagnetic - a quick on-site magnet test distinguishes it from 316L.

Physical properties, annealed, 20 C

Property

2205

316L (reference)

Density

7.8 g/cm3

8.0 g/cm3

Elastic modulus

200 GPa

195 GPa

Thermal expansion (20-100 C)

~13.0 x 10^-6 /K

~16.0 x 10^-6 /K

Thermal conductivity

~19 W/m-K

~15 W/m-K

Electrical resistivity

~0.80 uohm-m

~0.74 uohm-m

Magnetic

Ferromagnetic

Non-magnetic (austenitic)

The lower thermal expansion and higher conductivity are practical bonuses: 2205 tracks carbon steel better in mixed piping, and it dissipates heat faster in exchanger service. The magnetism lets inspectors confirm grade with a simple magnet - 2205 clings, 316L does not.

Which Standards and Equivalent Grades Cover Duplex 2205?

2205 is covered by ASTM A789 (tubing), A790 (pipe), A240 (plate/sheet/strip), A276 and A479 (bar), A182 F60 (flanges) and A815 (fittings). Its European grade is EN 1.4462 (Werkstoff 1.4462); the common forged grade codes are F60 for S32205 and F51 for S31803.

Common standards and equivalents for Duplex 2205

Product form

ASTM / ASME

UNS

European / other

Seamless & welded pipe

A790 / SA790

S32205, S31803

EN 10216-5 (1.4462)

Tubing

A789 / SA789

S32205, S31803

EN 10216-5

Plate, sheet, strip

A240 / SA240

S32205, S31803

EN 10088-2 (1.4462)

Bar (forging & general)

A276, A479

S32205, S31803

EN 10088-3

Flanges

A182 F60 / F51

S32205 / S31803

EN 1092

Fittings

A815 / SA815

S32205, S31803

EN 10253

Forged grade code

F60 (S32205)

F51 (S31803)

1.4462

When you see "F60" on a flange drawing or "1.4462" on a European spec, you are looking at the same material family as UNS S32205. Our ASTM A182 F60 flange page covers the forged form in detail.

In What Product Forms Is Duplex 2205 Available?

2205 is produced as seamless and welded pipe and tube, plate and sheet, round and flat bar, forged flanges and a full range of butt-welding fittings, so it can be sourced for almost any pressure-equipment or structural component.

Because the grade is weldable and formable with correct procedure, fabricators use it for everything from line pipe and heat-exchanger tubing to pressure-vessel shells, shafts, fasteners and structural members. Choose the form that matches the part:

  • Pipe and tube - Duplex 2205 pipe per ASTM A790 / A789, seamless or welded, annealed and pickled.

  • Plate and sheet - Duplex 2205 plate per ASTM A240 for vessels and structural work.

  • Bar - Duplex 2205 round bar per A276 / A479 for shafts, fasteners and machined parts.

  • Flanges and fittings - A182 F60 flanges and A815 fittings for complete piping assemblies.

Which Industries Use Duplex 2205?

2205 dominates offshore topsides, oil and gas flowlines, desalination, chemical processing, pulp and paper, and marine structural work - anywhere chlorides and strength together rule out 316L but full super duplex is not yet justified.

Which Industries Use Duplex 2205.webp

The driver in nearly every case is the combination of chloride resistance and high strength at a manageable cost. In desalination and seawater handling, 2205 is the workhorse for piping and structural members up to moderate temperatures; in oil and gas it serves both sweet and sour production systems. For a deeper look at the higher-grade end of the same problem, our Super Duplex S32750 seawater desalination guide shows where 2507 is specified instead.

  • Offshore and marine - topside piping, seawater lift, firewater systems.

  • Oil and gas - flowlines, risers, separators, sour-service headers.

  • Desalination - SWRO and MSF plant piping and structures.

  • Chemical and petrochemical - heat exchangers, tanks, process piping.

  • Pulp and paper - digesters and bleaching equipment (chloride + heat).

What Is the Allowable Service Temperature Range?

Use 2205 from about -50 C up to roughly 300 C continuous. Avoid prolonged exposure in the 280-520 C band, where 475 C embrittlement and sigma-phase precipitation can badly degrade toughness and corrosion resistance.

The duplex structure is stable only across a defined temperature window. Below about -50 C the impact toughness margin narrows (still acceptable, but verify for cryogenic duty). Above 300 C the strength falls and, critically, the ferrite phase begins to precipitate hard, brittle intermetallic phases. Short excursions during welding are managed by fast cooling; long holds in service are not.

Service-temperature envelope for 2205

Range

Condition

Note

-50 C to 300 C

Normal continuous service

Full properties apply

280-520 C

Avoid prolonged exposure

475 C embrittlement + sigma phase

> 300 C sustained

Strength derate

Use ASME Section II Part D elevated-temp values

600-1000 C

Never hold here

Severe intermetallic precipitation

Is Duplex 2205 Suitable for Sour (H2S) Service?

Yes. 2205 is qualified for H2S service under NACE MR0175 / ISO 15156-3 provided the parent metal hardness stays around 28 HRC maximum and the ferrite balance is verified - making it a standard choice for sour oil and gas production where carbon steel would fail by sulfide stress cracking.

Qualification is conditional, not automatic. The standard requires the duplex to be in the correct phase balance and below the hardness ceiling, and it restricts the partial pressures of H2S and the chloride level by temperature. A properly annealed and certified 2205 heat meets these conditions routinely, which is why it appears so often in sour-production specifications. See our duplex FAQ for the common sour-service questions.

How Is Duplex 2205 Welded?

Weld 2205 with overalloyed ER2209 / E2209 filler, keep interpass temperature at 150 C maximum, and do not post-weld heat treat. The joint must cool quickly through the precipitation range so the ferrite-austenite balance - and therefore the corrosion resistance - is preserved in the weld and heat-affected zone.

Duplex welding is more demanding than welding 316L because the weld metal and HAZ must return to the 40-60 percent ferrite balance on cooling. Use enough heat input to avoid a fully ferritic, brittle weld, but not so much that the joint soaks in the dangerous temperature band. Control is achieved with interpass limits, controlled heat input and, for critical joints, a restricted root-gas environment. Our duplex and super duplex overview carries the fabrication detail.

Parameter

Recommended practice

Filler metal

ER2209 / E2209 (overalloyed duplex)

Interpass temperature

150 C maximum

Heat input

Controlled; avoid both too-low and too-high

Post-weld heat treatment

None (do not stress-relieve)

Root shielding

Argon purge for critical joints

Ferrite check

Measure weld metal ferrite on procedure coupon

Why Are Phase Balance and Heat Treatment Critical?

Because 2205 is a phase-balanced alloy, any slow cooling through 280-520 C or improper anneal can precipitate sigma or chi phase and destroy corrosion resistance. That is why solution annealing at 1040-1100 C with rapid quench, plus ASTM A923 verification, is mandatory for demanding service.

The annealing step dissolves any intermetallic phases and re-establishes the 50/50 structure; the rapid quench locks it in. If a fabricator anneals too cold, or cools too slowly, sigma phase forms at ferrite grain boundaries and the material loses both toughness and pitting resistance - often with no visible warning. ASTM A923 (Method A etching, B charpy, C microscopy) is the standard check for these deleterious phases.

If a supplier cannot show ASTM A923 (or equivalent) verification for a 2205 heat in seawater or sour duty, treat the material as unproven - the alloy's whole advantage lives in its phase balance.

How Can You Verify a Genuine Duplex 2205 Heat?

Confirm a genuine 2205 heat with positive material identification (PMI), ferrite measurement, an ASTM A923 intermetallic-phase test, and - for seawater or sour duty - ASTM G48 Method A pitting (CPT) verification, all traceable to an EN 10204 3.1 or 3.2 certificate.

Verification is layered: PMI with XRF confirms the chemistry matches UNS S32205; the ferrite scope or ASTM E562 confirms the 40-60 percent balance; A923 confirms no harmful intermetallics; and G48 Method A measures the actual critical pitting temperature. Together they catch both grade substitution and poor heat treatment - the two failure modes that matter for 2205. General duplex questions are answered in our FAQ list.

Recommended verification tests

Test

Standard

What it proves

PMI (XRF/OES)

Mill + site check

Grade and chemistry match

Ferrite

Ferritescope / ASTM E562

40-60% phase balance

Intermetallic phase

ASTM A923 A/B/C

No sigma/chi phase

Pitting

ASTM G48 Method A

Actual CPT in chloride

Mechanical

ASTM A370

Yield, tensile, elongation, hardness

How Does Duplex 2205 Compare with Super Duplex 2507 (S32750)?

Super Duplex 2507 (UNS S32750) is the logical upgrade from 2205: higher chromium (24-26 percent), more nickel and molybdenum, and nitrogen near 0.25 percent lift its PREN to about 38-42 and yield to 550 MPa. Choose 2507 when chloride exceeds roughly 10,000 ppm, seawater temperature rises above about 35 C, or design margins demand it.

Duplex 2205 Compare with Super Duplex 2507.webp

The two grades share the same dual-phase philosophy, so 2507 is not a different technology but a more heavily alloyed member of the same family. That continuity is useful: the welding and phase-balance discipline you apply to 2205 carries directly to 2507. For the complete picture, start with what Super Duplex S32750 is, then read our Ultimate Guide to Super Duplex S32750, which this article supports as part of the S32750 content hub.

2205 vs Super Duplex 2507 (S32750)

Property

Duplex 2205 (S32205)

Super Duplex 2507 (S32750)

Chromium

22.0-23.0%

24.0-26.0%

Nickel

4.5-6.5%

6.0-8.0%

Molybdenum

3.0-3.5%

3.0-5.0%

Nitrogen

0.14-0.20%

0.24-0.32%

PREN

34-38

38-42

Yield, min

450 MPa (65 ksi)

550 MPa (80 ksi)

Tensile, min

620-655 MPa

795 MPa (116 ksi)

Best use

Topside, moderate chloride

Hot seawater, high chloride, subsea

What Are the Limitations of Duplex 2205?

2205 is not a high-temperature grade, is only moderately resistant in hot concentrated chloride, and is more fabrication-sensitive than 316L. Step up to Super Duplex 2507 when chloride, temperature or design margins exceed its envelope.

Three limits recur in practice. First, the 300 C continuous ceiling rules it out for hot sections where 316L (oxidation-limited) would still serve. Second, in hot concentrated chloride or strong acid it eventually pits where 2507 or a nickel alloy is needed. Third, it demands disciplined welding and heat treatment - a shop that treats it like 316L will produce embrittled or sensitized joints. A direct comparison is in 2205 vs 2507: when to use which.

  • Temperature: not for sustained service above ~300 C.

  • Hot concentrated chloride: 2507 or a nickel alloy performs better.

  • Fabrication: requires controlled welding and verified heat treatment.

  • Thick sections: slower cooling can drift ferrite balance - verify per heat.

How Should You Specify Duplex 2205 in a Purchase Order?

A complete specification names the UNS, the product standard and form (for example ASTM A790 UNS S32205 pipe, solution-annealed and pickled), the required ferrite band, the inspection level and the EN 10204 certificate type.

Vague orders such as "duplex pipe" invite the wrong grade or the wrong heat treatment. Pin down the designation, the delivery condition, the ferrite range you will accept, and the test reports you require (PMI, ferrite, A923, G48 as applicable). For pipe specifically, our ASTM A790 S31803/S32205 pipe page lists the dimensions, schedules and tolerances to reference.

  • Grade: UNS S32205 (preferred) per ASTM A789/A790/A240 as applicable.

  • Condition: solution-annealed and pickled; specify surface finish if needed.

  • Ferrite: 40-60% (target 45-55%) with measurement report.

  • Inspection: PMI, A923 (seawater/sour), G48 Method A CPT if specified.

  • Certificate: EN 10204 3.1 or 3.2 with full heat analysis.

Where Can You Source Certified Duplex 2205 Products?

Source certified 2205 from a supplier that provides full duplex-specific documentation and project references. JN Alloy stocks Duplex 2205 pipe, plate and bar with the inspection package described above and can support both standard and custom requirements.

Certified Duplex 2205 Products.webp

Beyond the material itself, the differentiator is traceability and verification: a documented heat, a ferrite report, and a supplier track record in duplex fabrication. Review a relevant shipped project such as our UNS S32750 butt-welding fittings shipped to Saudi Arabia to see how duplex-family orders are handled end to end. For stock and forms, visit JN Alloy Duplex 2205.

Key Facts About Duplex 2205 Stainless Steel

What Duplex 2205 is

A dual-phase (austenitic-ferritic) stainless steel whose annealed microstructure is about 50 percent ferrite and 50 percent austenite. UNS S32205 (and the older S31803) is the grade; EN 1.4462 is the European designation. See the duplex numbering system for how the UNS and EN codes relate.

The single number that defines it

The '2205' label is the market name tied to the original 22 percent chromium / 5 percent nickel balance. Today the controlling chemistry is UNS S32205: 22.0-23.0 percent chromium, 4.5-6.5 percent nickel, 3.0-3.5 percent molybdenum, 0.14-0.20 percent nitrogen.

Pitting resistance equivalent

PREN = percent Cr + 3.3 x percent Mo + 16 x percent N. For 2205 that lands at roughly 34-38, versus about 24-26 for 316L - a step that turns chloride pitting from 'likely' to 'managed'.

Strength that halves the wall

Minimum yield is 450 MPa (65 ksi), about 2.6 times that of 316L (170 MPa). For the same pressure and diameter, a 2205 shell can be roughly 30-50 percent thinner, cutting both weight and material cost even though the alloy itself costs more per kilogram.

Ferrite balance is not optional

ASTM A790 / A789 require 35-65 percent ferrite after solution annealing; most mills target 45-55 percent. Outside that band the alloy loses the very properties that justify using it. Duplex FAQ covers how it is measured.

Temperature ceiling

Continuous service is normally limited to about 300 C. Between roughly 280 C and 520 C the ferrite phase can form brittle sigma phase and 475 C embrittlement, so 2205 is a room-temperature-to-moderate-heat material, not a high-temperature grade.

Sour-service qualification

2205 is listed in NACE MR0175 / ISO 15156-3 for H2S environments subject to hardness and microstructure limits. Parent-metal hardness is normally held at or below about 28 HRC, with the ferrite fraction verified on the certificate.

When 2205 is not enough

Step up to Super Duplex 2507 (UNS S32750) when chloride exceeds about 10,000 ppm, seawater temperature rises above roughly 35 C, or you need higher design margins. Our Super Duplex S32750 guide explains the boundary in detail.

Frequently Asked Questions

What is Duplex 2205 stainless steel?

Duplex 2205 is a dual-phase (austenitic-ferritic) stainless steel whose annealed structure is about 50 percent ferrite and 50 percent austenite. Its primary grade is UNS S32205 and the European equivalent is EN 1.4462. It offers roughly twice the yield strength of 316L with much better resistance to chloride pitting and stress-corrosion cracking.

Is 2205 the same as 316 stainless steel?

No. 316 is fully austenitic, while 2205 is a two-phase duplex alloy. 2205 has about 2.6 times the yield strength of 316L (450 MPa vs 170 MPa) and a PREN of 34-38 versus 24-26 for 316L, so it resists chloride attack far better but is more sensitive to fabrication temperature.

What does UNS S32205 mean?

UNS stands for Unified Numbering System. S32205 is the active duplex grade with 22.0-23.0 percent chromium, 3.0-3.5 percent molybdenum and 0.14-0.20 percent nitrogen. The older S31803 is still valid but has a wider chromium range and lower nitrogen.

What is the difference between S31803 and S32205?

Both are Duplex 2205. S32205 has a tighter chromium range (22.0-23.0 percent vs 21.0-23.0 percent) and higher minimum nitrogen (0.14 percent vs 0.08 percent). Most new specifications call for S32205 because it gives more consistent phase balance and corrosion resistance.

What does 2205 stand for?

The name comes from the original nominal composition: about 22 percent chromium and 5 percent nickel. Modern S32205 tolerances are tighter, but the family name has stuck.

What is EN 1.4462?

EN 1.4462 is the European designation for Duplex 2205, equivalent to UNS S32205 / S31803. You will see it on European material certificates and EN standards such as EN 10088 and EN 10216-5.

What is the PREN of Duplex 2205?

PREN equals percent Cr + 3.3 x percent Mo + 16 x percent N. For 2205 that gives about 34-38, versus 24-26 for 316L. The higher PREN means pitting starts at a higher temperature in chloride service.

Why is nitrogen important in 2205?

Nitrogen is a strong austenite stabilizer and a powerful strengthener; it also boosts PREN and slows the formation of brittle sigma phase during welding. The 0.14-0.20 percent nitrogen in S32205 is what lets the grade hold its phase balance and high strength.

What is the yield strength of Duplex 2205?

The minimum yield strength is 450 MPa (65 ksi) and tensile is 620-655 MPa (90-95 ksi) in the solution-annealed condition. Typical mill values are often higher, but design should use the minimum.

What is the ferrite content of 2205?

ASTM A789/A790 require 35-65 percent ferrite after solution annealing; most mills target 45-55 percent. This balance is what gives 2205 its combination of strength, toughness and chloride stress-corrosion resistance.

Is Duplex 2205 magnetic?

Yes. Because roughly half the structure is ferrite, 2205 is ferromagnetic, unlike fully austenitic 316L. A simple magnet test helps distinguish 2205 from 316L on site.

What temperature range can 2205 withstand?

Use it from about -50 C up to roughly 300 C continuous. Avoid prolonged exposure between 280 C and 520 C, where 475 C embrittlement and sigma phase can form and degrade properties.

Can Duplex 2205 be used in high-temperature service?

Not as a high-temperature alloy. Above about 300 C its strength derates and it risks intermetallic precipitation. For sustained high heat, choose a stabilized or high-nickel grade instead.

Is 2205 suitable for seawater?

Yes for topside and moderate-temperature seawater, which is a major application. In hot seawater or above about 10,000 ppm chloride, Super Duplex 2507 (S32750) is usually specified instead. See our Super Duplex S32750 guide.

Is Duplex 2205 good for sour (H2S) service?

Yes, 2205 is listed in NACE MR0175 / ISO 15156-3 for H2S service subject to hardness and microstructure limits (parent hardness around 28 HRC maximum and verified ferrite balance).

What is NACE MR0175 / ISO 15156?

These are the international standards that define which materials may be used in sour (H2S-containing) oil and gas service and under what conditions. 2205 qualifies provided its hardness and phase balance stay within the limits.

What welding filler is used for 2205?

Use overalloyed duplex filler ER2209 / E2209. The goal is to keep the weld metal in the correct ferrite-austenite balance and resistant to pitting.

What interpass temperature is allowed when welding 2205?

Keep interpass temperature at 150 C maximum. Too much heat lets the joint linger in the precipitation range and can form sigma phase.

Can 2205 be post-weld heat treated?

Generally no. Do not stress-relieve or anneal after welding in the 280-520 C range; it would embrittle the joint. If a heat treatment is required, it must be a full solution anneal at 1040-1100 C followed by rapid quench.

What is the proper heat treatment for 2205?

Solution anneal at 1040-1100 C followed by rapid quench (water or fast air). This dissolves any intermetallic phases and restores the 50/50 structure.

What is sigma phase in duplex stainless steel?

Sigma phase is a hard, brittle intermetallic compound that can precipitate in the ferrite at 280-520 C. It reduces toughness and pitting resistance. ASTM A923 detects it, and correct annealing plus fast cooling prevents it.

How do you test Duplex 2205 quality?

Use PMI to confirm chemistry, a ferritescope or ASTM E562 for ferrite balance, ASTM A923 for intermetallic phases, and (for seawater or sour duty) ASTM G48 Method A for pitting. All should tie back to an EN 10204 certificate.

What standards cover Duplex 2205 pipe?

ASTM A789 covers tubing and A790 covers pipe (ASME SA789/SA790 for Code use). Plate is A240, bar is A276/A479, flanges are A182 F60, and fittings are A815.

What is F60 in duplex stainless steel?

F60 is the ASME/ASTM forged grade designation for UNS S32205 (F51 is the older S31803). You will see F60 on flange and forging drawings.

When should I choose 2205 instead of Super Duplex 2507?

Choose 2205 when chloride, temperature and design margins are moderate - typically below about 10,000 ppm chloride and below roughly 35 C seawater. Step up to 2507 when those limits are exceeded. Our 2205 vs 2507 guide gives the decision rules.

Is Duplex 2205 more expensive than 316L?

Yes per kilogram, because of higher alloy content, but its higher strength allows thinner walls, so on a finished component the cost penalty is often smaller than the material price gap suggests.

Glossary

Duplex stainless steel

A stainless steel with a mixed austenitic-ferritic microstructure, typically near 50/50 in the annealed condition.

Austenite

The face-centred-cubic, non-magnetic phase that gives stainless steel toughness and ductility.

Ferrite

The body-centred-cubic, magnetic phase that gives duplex steel its strength and resistance to chloride stress-corrosion cracking.

UNS S32205

The active Duplex 2205 designation, with chromium 22.0-23.0 percent, molybdenum 3.0-3.5 percent and nitrogen 0.14-0.20 percent.

UNS S31803

The original Duplex 2205 designation, still valid, with a wider chromium range and lower minimum nitrogen than S32205.

EN 1.4462

The European grade number for Duplex 2205, equivalent to UNS S32205 / S31803.

F60 / F51

Forged grade codes: F60 = UNS S32205, F51 = UNS S31803.

PREN

Pitting Resistance Equivalent Number, calculated as %Cr + 3.3 x %Mo + 16 x %N; higher means better pitting resistance.

CPT

Critical Pitting Temperature, the threshold at which pitting begins in a chloride solution; measured by ASTM G48.

CCT

Critical Crevice Temperature, the analogous threshold for crevice corrosion.

Sigma phase

A hard, brittle intermetallic phase that precipitates at 280-520 C and degrades toughness and corrosion resistance.

475 C embrittlement

Brittleness that develops in the ferrite phase after prolonged exposure near 475 C; a key reason 2205 has a 300 C service ceiling.

Solution annealing

Heating to 1040-1100 C and rapidly quenching to dissolve intermetallic phases and restore the duplex structure.

Interpass temperature

The maximum temperature of the previous weld pass before the next is deposited; kept at 150 C max for 2205.

ER2209 / E2209

The overalloyed duplex filler metals used to weld 2205.

NACE MR0175 / ISO 15156

Standards governing material use in sour (H2S-containing) oil and gas service.

ASTM A789

Specification for seamless and welded ferritic/austenitic duplex tubing.

ASTM A790

Specification for seamless and welded duplex pipe.

ASTM A240

Specification for duplex plate, sheet and strip.

ASTM A182 F60

Specification for forged duplex flanges and fittings (F60 = S32205).

ASTM A815

Specification for wrought duplex butt-welding fittings.

ASTM A923

Test methods for detecting detrimental intermetallic phases in duplex stainless steels.

ASTM E562

Standard practice for determining volume fraction of ferrite by systematic manual point count.

PMI

Positive Material Identification, usually XRF or OES, used to confirm grade and chemistry on site.

EN 10204 3.1 / 3.2

Material certificate types: 3.1 is a declaration by the manufacturer, 3.2 adds independent verification.

Super Duplex 2507

UNS S32750, a more heavily alloyed duplex grade (PREN 38-42) used where 2205 is insufficient; see S32750 guide.

References & Standards

  1. ASTM A789 / ASME SA789 - Standard Specification for Seamless and Welded Ferritic/Austenitic Stainless Steel Tubing for General Service.

  2. ASTM A790 / ASME SA790 - Standard Specification for Seamless and Welded Ferritic/Austenitic Duplex Stainless Steel Pipe.

  3. ASTM A240 / ASME SA240 - Standard Specification for Chromium and Chromium-Nickel Stainless Steel Plate, Sheet and Strip for Pressure Vessels.

  4. ASTM A276 - Standard Specification for Stainless Steel Bars and Shapes.

  5. ASTM A479 - Standard Specification for Stainless Steel Bars and Shapes for Use in Boilers and Other Pressure Vessels.

  6. ASTM A182 / ASME SA182 - Standard Specification for Forged or Rolled Alloy and Stainless Steel Pipe Flanges (F60 = S32205).

  7. ASTM A815 / ASME SA815 - Standard Specification for Wrought Ferritic, Ferritic/Austenitic and Martensitic Stainless Steel Piping Fittings.

  8. EN 10088-1 / -2 / -3 - European stainless steel standards covering general properties, plate/sheet and bar (EN 1.4462 = Duplex 2205).

  9. EN 10216-5 - Seamless steel tubes for pressure purposes: stainless steel tubes.

  10. EN 1092 - Flanges and their joints: circular flanges for pipes, valves and fittings (PN designated).

  11. ASTM A923 - Standard Test Methods for Detecting Detrimental Intermetallic Phase in Duplex Stainless Steels.

  12. ASTM A480 / A480M - General requirements for flat-rolled stainless steel plate, sheet and strip.

  13. ASTM G48 - Standard Test Methods for Pitting and Crevice Corrosion Resistance of Stainless Steels and Related Alloys by Use of Ferric Chloride Solution (Method A = CPT).

  14. ASTM E562 - Standard Practice for Determining Volume Fraction by Systematic Manual Point Count.

  15. NACE MR0175 / ISO 15156 - Petroleum and natural gas industries - Materials for use in H2S-containing environments in oil and gas production (Part 3 covers duplex stainless steels).

  16. NORSOK MDS D36 - Material data sheet for duplex stainless steel (S32205) in offshore service.

  17. ASME Boiler and Pressure Vessel Code, Section II Part D - Allowable stresses and physical properties for S32205 at design temperatures.

  18. ASME BPVC Section IX - Qualification of welding procedure and performance for duplex base and filler metals.

  19. AWS A4.2 - Standard Procedure for Calibrating Magnetic Instruments to Measure the Delta Ferrite Content of Austenitic and Duplex Ferritic-Austenitic Weld Metal.

  20. WRC-1992 Diagram - Weld metal ferrite prediction diagram used to target the correct ferrite number in duplex welds.

  21. EN 10204 - Metallic products - Types of inspection documents (3.1 and 3.2 certificates).

  22. ASTM A370 - Standard Test Methods and Definitions for Mechanical Testing of Steel Products.

  23. ASTM A999 / A999M - General requirements for alloy and stainless steel pipe.

  24. ISO 9328 / EN 10028 - Plate standards referenced for duplex pressure-equipment plate supply.

  25. ASTM A988 - Standard Specification for Hot Isostatically Pressed stainless steel duplex forgings (related duplex supply route).

  26. JN Alloy technical data - Duplex 2205 product forms: pipe, plate, round bar.

Need certified Duplex 2205 (UNS S32205 / EN 1.4462) pipe, plate or bar with EN 10204 3.1 material certification, ferrite balance 40-60 percent and ASTM A923 intermetallic-phase verification? Browse our Duplex 2205 pipe, Duplex 2205 plate and Duplex 2205 round bar, or send your specification to JN Alloy for a full quotation. If your service exceeds hot seawater or 10,000 ppm chloride, also see our Ultimate Guide to Super Duplex S32750 (2507) to confirm the right grade.

content is empty!

For extreme operating conditions, choose JINIE; for high-end manufacturing, rely on JINIE.
A one-stop solution for:
Difficulties in material selection, processing, inspection, and after-sales support.
Tel: +86 19339900211
Add: Shuangchuang Building, High-tech Industrial Development Zone, Lu'an City, Anhui Province, China
Copyright © ANHUI JINIE SPECIAL ALLOY CO.,LTD. All Rights Reserved.