S32750 and S32760 are the two standard super duplex stainless steels, sold as F53 and F55 for forgings and flanges. They share the same 24-26% chromium, 6-8% nickel platform and the same 550 MPa yield strength, so for most seawater and chloride duty they are effectively interchangeable. The engineering difference is small but real: S32760 adds tungsten and copper, while S32750 carries more molybdenum and nitrogen.

S32750 vs S32760.webp

This guide works through every difference and tells you when each is the right call - part of the Super Duplex S32750 hub.

What is the difference between S32750 and S32760?

S32750 and S32760 are sister super duplex grades built on the same 25Cr-7Ni-4Mo platform: S32760 (F55) adds tungsten and copper, while S32750 (F53) keeps more molybdenum and nitrogen - so F55 wins in reducing acids and F53 wins on chloride pitting and tensile strength.

Both are roughly 50/50 austenite-ferritic stainless steels with a PREN above 40, which is what puts them in the super duplex class rather than standard duplex. In practice the two are often treated as interchangeable, and for continuous seawater or neutral chloride service they genuinely are.

The differences that matter show up in three places: reducing acids, where S32760's copper helps; pitting margin, where S32750's higher molybdenum and nitrogen give it a higher critical pitting temperature; and tensile strength, where S32750 is listed at 795 MPa against 750 MPa for S32760.

If you are new to the family, start with What Is Super Duplex S32750? for the background, or read the S32760 overview for the F55 side. The rest of this article compares them property by property.

Which UNS, EN and trade names identify each grade?

S32750 is UNS S32750, forge grade F53, EN 1.4410, sold as SAF 2507; S32760 is UNS S32760, forge grade F55, EN 1.4501, sold as Zeron 100 - and the trade names are exactly the same alloys, not superior versions.

Procurement documents should always carry the UNS number, because trade names and national codes vary by supplier while the UNS number is unique. The F53 and F55 designations are the forge-grade codes used under ASTM A182, so a flange drawing marked F53 means UNS S32750.

UNS number

S32750

S32760

ASTM A182 forge grade

Grade F53

Grade F55

EN / DIN material number

1.4410

1.4501

EN steel name

X2CrNiMoN25-7-4

X2CrNiMoCuWN25-7-4

Trade name

SAF 2507 (Sandvik)

Zeron 100 (Rolled Alloys)

Chinese GB designation

022Cr25Ni7Mo4N

022Cr25Ni7Mo4WCuN

Our page on the duplex stainless steel numbering system explains how UNS, ASTM, EN and GB codes map onto each other, which removes most of the confusion when quoting a mixed specification.

How does the chemical composition of S32750 compare with S32760?

Chromium and nickel are identical at 24-26% and 6-8%; the differences are that F53 allows more molybdenum (3-5% vs 3-4%) and more nitrogen (0.24-0.32% vs 0.20-0.30%), while F55 adds copper (0.5-1.0%) and tungsten (0.5-1.0%).

How does the chemical composition of S32750 compare with S32760.webp

These four elements explain almost every performance difference between the grades. Molybdenum and nitrogen drive the pitting-resistance number, which is why F53 holds a higher guaranteed PREN and a higher critical pitting temperature. Copper is the classic addition for reducing acids, giving F55 its edge in sulfuric and hydrochloric acid. Tungsten behaves like molybdenum in localized attack, which is why the W-inclusive PREN formula (PREN-W) brings the two grades back onto level terms.

Chromium (Cr)

24.0 - 26.0

24.0 - 26.0

Primary pitting and oxidation barrier

Nickel (Ni)

6.0 - 8.0

6.0 - 8.0

Austenite stabiliser and toughness

Molybdenum (Mo)

3.0 - 5.0

3.0 - 4.0

Pitting and crevice resistance

Nitrogen (N)

0.24 - 0.32

0.20 - 0.30

Strength and PREN contribution

Copper (Cu)

0.50 max

0.50 - 1.00

F55's reducing-acid advantage

Tungsten (W)

not specified

0.50 - 1.00

Localized attack resistance

Carbon (C)

0.030 max

0.030 max

Low to avoid sensitisation

Silicon (Si)

0.80 max

1.00 max

Deoxidiser

Manganese (Mn)

1.20 max

1.00 max

Minor austenite stabiliser

Which grade has the higher mechanical strength?

Yield strength is identical at 550 MPa (80 ksi) minimum for both grades; S32750 is listed with the higher tensile strength at 795 MPa (115 ksi) against 750 MPa (109 ksi) for S32760.

For pressure-vessel and piping design the yield strength is the number that drives wall thickness, and both grades give you the same 550 MPa - about three times 316L and about 20% above Duplex 2205. The tensile difference is real but small in practice, and elongation, reduction of area, hardness and Charpy requirements are the same for both grades under ASTM A182.

Property

F53 (S32750)

F55 (S32760)

Standard

0.2% proof (yield)

550 MPa (80 ksi)

550 MPa (80 ksi)

ASTM A182

Ultimate tensile

795 MPa (115 ksi)

750 MPa (109 ksi)

ASTM A182

Elongation

25% min

25% min

ASTM A182

Reduction of area

45% min

45% min

ASTM A182 / EN 10088

Hardness

32 HRC / 310 HBW max

32 HRC / 310 HBW max

ASTM A182

Charpy at 0 degC (transverse)

27 J min (typical 60-80 J)

27 J min (typical 60-80 J)

EN ISO 148-1

Elastic modulus

about 196 GPa

about 196 GPa

Reference data

Always confirm the governing specification edition and product form before using these numbers for design - our S32750 properties page carries the same values alongside corrosion data.

Are the physical properties of S32750 and S32760 the same?

Yes - density, elastic modulus, thermal conductivity, thermal expansion, resistivity and specific heat are effectively identical, so weight, stiffness and thermal calculations do not distinguish the two grades.

The small tungsten and copper additions in F55 do not move the physical properties enough to matter for design. A flange in F53 and the same flange in F55 weigh the same to the first decimal place, and both expand at 13.0 microstrain per degree C over 20-100 degC.

Property

F53 (S32750)

F55 (S32760)

Unit

Density

7.80

7.80

g/cm3

Elastic modulus at 20 degC

about 196

about 196

GPa

Thermal conductivity at 20 degC

about 14

about 14

W/m-K

Mean thermal expansion 20-100 degC

13.0

13.0

x10-6 /degC

Electrical resistivity at 20 degC

about 0.80

about 0.80

microohm-m

Specific heat capacity

about 480

about 480

J/kg-K

Maximum service temperature

300

300

degC

Which grade resists pitting corrosion better?

S32750 holds the higher critical pitting temperature in ASTM G48-C testing (above 50 degC against above 40 degC for S32760), thanks to its higher molybdenum and nitrogen - but both are far beyond 316L and Duplex 2205.

Critical pitting temperature is the temperature at which pitting starts in a standard ferric chloride test, and it is the cleanest single measure of pitting resistance. F53's higher molybdenum ceiling and higher nitrogen range push its CPT above 50 degC. F55 still clears 40 degC, which is excellent in absolute terms. Critical crevice temperature is the same for both at above 25 degC, and both resist chloride stress-corrosion cracking far better than any austenitic grade.

Corrosion parameter

F53 (S32750)

F55 (S32760)

Remark

PREN (Cr + 3.3Mo + 16N)

above 41

40 guaranteed min

Standard formula

PREN-W (W-inclusive)

about 41 - 43

about 41 - 42

Tungsten lifts F55

Critical pitting temp (ASTM G48-C)

above 50 degC

above 40 degC

In 6% FeCl3

Critical crevice temp (ASTM G48-D)

above 25 degC

above 25 degC

316L is about 10 degC

Chloride stress-corrosion cracking

Excellent

Excellent

Both far exceed 316L and 2205

Reducing acids (H2SO4, HCl)

Good

Superior

Copper in F55 is decisive

Seawater and brine

Excellent

Excellent

Interchangeable

H2S sour service

Qualified

Qualified

NACE MR0175 / ISO 15156

Oxidising acids (nitric)

Good

Good

Not the primary choice

What is PREN, and why is F53's guaranteed value higher?

PREN = %Cr + 3.3x%Mo + 16x%N; because F53 allows more molybdenum and nitrogen than F55, its guaranteed PREN is above 41 while F55 is guaranteed at 40 - but adding tungsten in the PREN-W formula brings the two grades back to roughly the same level.

This is the single most misunderstood point in the comparison, because suppliers quote both formulas. The standard PREN formula ignores tungsten, so it favours F53. The W-inclusive formula, PREN-W = %Cr + 3.3x(%Mo + 0.5x%W) + 16x%N, credits F55's tungsten and puts both grades at roughly 41-43. Neither number is a design allowable; both are screening indices.

The honest summary is that the two grades sit at effectively the same pitting level, with F53's advantage concentrated in the ferric-chloride pitting test and F55's advantage concentrated in reducing acids.

Which grade is better for reducing acids like sulfuric and hydrochloric acid?

S32760 (F55) is the better choice in reducing acids - its 0.5-1.0% copper addition improves resistance to sulfuric and hydrochloric acid in a way molybdenum and nitrogen cannot.

Which grade is better for reducing acids like sulfuric and hydrochloric acid.webp

Copper has a long-established benefit in reducing-acid service on stainless steels, which is why F55 was developed. If the duty is acidic rather than simply chloride-rich - fertilizer plant lines, acid gas scrubbers, hydrometallurgical circuits - F55 is the more defensible selection. If the duty is seawater, brine or neutral chloride, the copper adds cost without adding performance and F53 is the better value.

Neither super duplex grade is a substitute for a nickel alloy in hot, concentrated acid. For sustained service in hot concentrated sulfuric or hydrochloric acid, step up to a nickel-base alloy such as Hastelloy C276 rather than trying to stretch either super duplex grade.

Which grade performs better in seawater and chloride service?

They are interchangeable in seawater, brine and neutral chloride duty - both clear the super duplex PREN threshold, resist chloride stress-corrosion cracking, and are qualified for sour service.

For desalination, offshore cooling water, splash zones and marine piping the choice should come down to availability and cost, not metallurgy. Our seawater desalination guide works through the specific equipment where the grade choice interacts with design, and the 2205 vs 2507 comparison covers the next step down if the environment is milder.

Can both grades be used in sour H2S service?

Yes - both S32750 and S32760 are qualified for sour service under NACE MR0175 / ISO 15156 when supplied solution-annealed, with hardness at or below 32 HRC and the specified ferrite balance.

That 32 HRC ceiling is also the same hardness limit listed in ASTM A182 for both forge grades, which is convenient: a single purchase requirement covers both the mechanical specification and the sour-service qualification. Confirm the temperature and H2S partial-pressure limits in the current edition of the standard for your exact environment, and keep the ferrite fraction inside the 40-60% window through qualified heat treatment and welding.

What is the maximum service temperature for S32750 and S32760?

Both grades are limited to about 300 degC (572 degF) of continuous stressed service, because the ferrite phase can precipitate brittle sigma and chi intermetallics above that range.

What is the maximum service temperature for S32750 and S32760.webp

The limit is metallurgical, not a code number. Between roughly 250 and 300 degC and above, the ferrite in duplex steel begins to decompose into intermetallic phases that embrittle the material and hurt corrosion resistance. Above the ceiling, the correct move is a nickel alloy - Inconel 625 or Hastelloy C276 - rather than either super duplex grade. Note that short excursions above the limit are tolerated in practice, but the design condition should stay inside it.

Which ASTM and EN standards cover each grade?

Both grades are covered by the same specification set - ASTM A182 for forgings and flanges, A276 and A479 for bar, A240 for plate, A789/A790 for pipe and tube - with the grade identified as F53 or F55, S32750 or S32760, and 1.4410 or 1.4501 in EN.

Specification

F53 (S32750)

F55 (S32760)

Scope

ASTM A182 / A182M

Grade F53

Grade F55

Forged fittings and flanges

ASTM A276 / A276M

Covered

Covered

Stainless steel bars

ASTM A479 / A479M

Covered

Covered

Bars for pressure vessels

ASTM A240 / A240M

S32750

S32760

Plate, sheet and strip

ASTM A789 / A790

Covered

Covered

Seamless and welded duplex tube

EN 10088-3

1.4410

1.4501

Bars, rods and wire

EN 10028-7

Covered

Covered

Flat products for pressure vessels

NACE MR0175 / ISO 15156

Qualified

Qualified

Sour service (H2S)

NORSOK M-650

Qualified

Qualified

Manufacturer qualification

ISO 15510

Covered

Covered

Chemical composition of stainless steels

How does welding differ between S32750 and S32760?

Both grades weld on the same qualified duplex procedures - matching filler, argon backing, controlled heat input and post-weld ferrite checks - with S32760's copper content calling for slightly tighter control against solidification cracking.

The welding risk in duplex steel is not the filler metal but the heat-affected zone: cool it too slowly or overheat it and the ferrite-austenite balance drifts and intermetallic phases precipitate. Copper slightly increases solidification-cracking sensitivity, so S32760 procedures usually specify tighter heat input limits and a lower dilution from the base metal. In every other respect - purge requirements, filler selection, interpass temperature and the ASTM A923 phase check - the two grades are welded the same way. The hub's dedicated welding spoke covers procedures and filler selection in full.

How do S32750 and S32760 compare with 316L and Duplex 2205?

Both super duplex grades roughly triple the yield strength of 316L and out-corrode it in chloride service, and both sit above Duplex 2205 on PREN and strength - so the choice between them only becomes relevant once the environment has already ruled out 316L and 2205.

Property

316L

Duplex 2205

S32750 (F53)

S32760 (F55)

PREN (typical)

24 - 26

34 - 38

above 41

40 min, about 41 with W

Yield strength MPa

170

450

550

550

Tensile strength MPa

485

655

795

750

Seawater suitability

Poor to fair

Good

Excellent

Excellent

Relative material cost

Low

Medium

High

High

For a full walk-through of the step down, our 2205 vs Super Duplex 2507 comparison and the 316L and Duplex 2205 grade pages give the detail.

When should you choose S32750 (F53)?

Choose S32750 when chloride pitting margin, tensile strength or cost matters most - seawater cooling, desalination, offshore piping and general chloride service.

  • Chloride-dominated service where the critical pitting temperature is the controlling parameter.

  • Thick-wall pressure equipment where the higher 795 MPa tensile strength and higher PREN give margin.

  • Cost-sensitive projects, since F53 is the more widely stocked and more competitively priced of the two.

  • Applications where reducing acids are absent, so F55's copper adds nothing.

Shipped examples include F53 weld-neck flanges to Argentina and S32750 butt-welding fittings to Saudi Arabia - both chloride-side duty where F53 is the natural specification.

When should you choose S32760 (F55)?

Choose S32760 when the service contains reducing acids - sulfuric, hydrochloric or acid gas mixtures - where its copper and tungsten additions pay for themselves.

  • Sulfuric and hydrochloric acid service at moderate concentration and temperature.

  • Acid gas and scrubber service where chloride and acid coexist.

  • Specifications written against UNS S32760 or EN 1.4501, or against NORSOK projects that stock F55.

  • Reducing-acid duty where 254 SMO or a nickel alloy would be over-specification and 316L inadequate.

Where the environment sits between the two grades, our S32760 technical overview and the S32760 material page give the F55-specific data.

Which product forms are available in each grade?

Both grades are supplied in the same forms - plate and sheet, pipe and tube, bar and rod, forgings, flanges and butt-welding fittings - each under its own ASTM specification.

How do you specify the correct grade on a purchase order?

Write the UNS number, the forge grade where applicable, the ASTM specification and the required tests on the purchase order - that combination leaves no room for a substitution between the two grades.

  1. Start from the environment, not the grade. List the acid type and concentration, chloride level, temperature, pH and whether the service is sour. Chloride-dominated service keeps both grades in play; reducing acids such as sulfuric or hydrochloric tilt the choice to S32760.

  2. Check the pressure and strength case. Both grades give 550 MPa minimum yield, so strength is rarely decisive - but S32750's higher 795 MPa tensile and higher critical pitting temperature give it the edge in thick-wall, high-chloride duty.

  3. Confirm the sour-service and temperature envelope. If H2S is present, place the order against NACE MR0175 / ISO 15156 and keep the hardness at or below 32 HRC. Confirm continuous service stays below about 300 degC, where both grades are limited by sigma and chi phases.

  4. Write the UNS and the forge grade on the order. Specify the UNS (S32750 or S32760) and, for forgings and flanges, the forge grade (F53 or F55) together with the ASTM specification - A182 for forged fittings and flanges, A240 for plate.

  5. Require phase-balance and corrosion testing. Ask for ASTM A923 intermetallic-phase detection, ferrite measurement inside the 40-60% window, and the applicable ASTM G48 pitting or crevice test so the delivered heat matches the grade you selected.

Where can you read more about super duplex grades?

The Super Duplex S32750 hub collects every supporting article on the family, from the background definition through composition, properties, corrosion resistance and applications.

Key Facts About S32750 vs S32760

S32750 identity

UNS S32750, forge grade F53, EN 1.4410, trade name SAF 2507

S32760 identity

UNS S32760, forge grade F55, EN 1.4501, trade name Zeron 100

Shared chemistry

Both 24-26% Cr and 6-8% Ni - the same super duplex platform

The real difference

F55 adds tungsten (0.5-1.0%) and copper (0.5-1.0%); F53 carries more molybdenum (3-5%) and nitrogen (0.24-0.32%)

Yield strength

550 MPa (80 ksi) minimum - identical in both grades

Tensile strength

795 MPa (115 ksi) for F53 vs 750 MPa (109 ksi) for F55

PREN

F53 guaranteed above 41; F55 guaranteed at or above 40, with tungsten lifting its W-inclusive value

Decisive factor

Reducing acids favour F55 (copper); chloride pitting and strength favour F53

Service ceiling

About 300 degC for both, set by sigma/chi phase formation

Sour service

Both qualified to NACE MR0175 / ISO 15156, 32 HRC max

Frequently Asked Questions

What is the difference between S32750 and S32760?

They are the two standard super duplex stainless steels. Both use 24-26% chromium and 6-8% nickel and both give 550 MPa minimum yield strength. S32760 (F55) adds 0.5-1.0% tungsten and 0.5-1.0% copper, while S32750 (F53) carries more molybdenum (3-5%) and more nitrogen (0.24-0.32%). F55 is better in reducing acids, F53 better on chloride pitting margin and tensile strength.

Are S32750 and S32760 interchangeable?

For seawater, brine and neutral chloride service, yes - both are super duplex with PREN above 40 and both resist chloride stress-corrosion cracking. They stop being interchangeable in reducing-acid service, where F55's copper matters, and in specifications that name one UNS number explicitly.

What do F53 and F55 mean?

F53 and F55 are the forge-grade designations used under ASTM A182. F53 is UNS S32750 and F55 is UNS S32760, so a flange drawing marked F53 or F55 is simply naming the same alloy in forged form.

Which grade has higher strength, S32750 or S32760?

Yield strength is identical at 550 MPa (80 ksi) minimum for both. S32750 has the higher tensile strength at 795 MPa (115 ksi) against 750 MPa (109 ksi) for S32760, so F53 holds a modest edge on ultimate strength.

Which grade has better corrosion resistance?

It depends on the environment. In chloride pitting S32750 leads with a critical pitting temperature above 50 degC against above 40 degC for S32760. In reducing acids such as sulfuric and hydrochloric acid, S32760 leads because of its copper. In seawater both are excellent and effectively equal.

Which grade is better for seawater and desalination?

Either one. Both are qualified for continuous seawater exposure and both are standard grades for desalination, offshore cooling water and splash zones. Choose on availability and cost rather than metallurgy.

Which grade is better for sulfuric or hydrochloric acid?

S32760 (F55). Its 0.5-1.0% copper addition improves resistance to reducing acids, which is the main reason F55 exists. Neither grade replaces a nickel alloy in hot concentrated acid.

What is PREN, and how does it differ between the two grades?

PREN = %Cr + 3.3x%Mo + 16x%N. F53 is guaranteed above 41 and F55 at or above 40, because F53 allows more molybdenum and nitrogen. The W-inclusive formula PREN-W = %Cr + 3.3x(%Mo + 0.5x%W) + 16x%N credits F55's tungsten and puts both grades at roughly 41-43.

What is the critical pitting temperature of each grade?

In ASTM G48-C testing in 6% ferric chloride, S32750 sits above 50 degC and S32760 above 40 degC. Critical crevice temperature in ASTM G48-D is above 25 degC for both, against roughly 10 degC for 316L.

What is the maximum service temperature for both grades?

About 300 degC (572 degF) of continuous stressed service. Above that the ferrite can precipitate brittle sigma and chi intermetallic phases, so high-temperature duty should move to a nickel alloy.

Are both grades qualified for sour H2S service?

Yes. Both S32750 and S32760 are listed under NACE MR0175 / ISO 15156 when supplied solution-annealed with hardness at or below 32 HRC and the specified ferrite balance. Confirm the temperature and H2S partial-pressure limits in the current edition.

Which ASTM standards cover both grades?

ASTM A182 for forgings and flanges (as F53 and F55), A276 and A479 for bar, A240 for plate and sheet, and A789 / A790 for pipe and tube. EN equivalents are 1.4410 and 1.4501 under EN 10088.

What are the trade names for these grades?

S32750 (F53) is sold as SAF 2507 by Sandvik, and S32760 (F55) as Zeron 100 by Rolled Alloys. These are the same alloys as the UNS numbers, not superior versions.

Can S32760 be substituted for S32750?

In most chloride service, yes, but only as an upgrade approved by the engineer of record. The reverse is not always safe, because dropping from F55 to F53 removes the copper that a reducing-acid duty may depend on. Always confirm against the governing specification.

Which grade is cheaper?

S32750 (F53) is generally the more widely stocked and more competitively priced of the two, because it is the higher-volume grade. F55 carries a premium for its tungsten and copper additions.

How do these grades compare with 316L and Duplex 2205?

Both super duplex grades roughly triple the yield strength of 316L and out-corrode it in chloride service, and both sit above Duplex 2205 on PREN and strength. The choice between the two super duplex grades only becomes relevant once the environment has already ruled out 316L and 2205.

Do the two grades have the same density and weight?

Yes. Both are about 7.80 g/cm3, with the same elastic modulus, thermal conductivity, thermal expansion and specific heat, so weight, stiffness and thermal calculations do not distinguish them.

Which grade should I use for my project?

Start from the environment. Seawater, brine or neutral chloride with cost pressure points to S32750. Sulfuric or hydrochloric acid, or acid-gas service, points to S32760. If sour service is involved, both qualify under NACE MR0175 with a 32 HRC hardness ceiling.

Glossary

Super duplex stainless steel

A duplex grade with PREN above 40. S32750 (F53) and S32760 (F55) are the two standard members.

Duplex microstructure

A roughly 50/50 mix of austenite and ferrite that gives the grade its combination of strength and corrosion resistance.

UNS number

The Unified Numbering System code that uniquely identifies an alloy - S32750 and S32760 here. The 'S' prefix denotes stainless steel.

F53 / F55

The ASTM A182 forge-grade designations for UNS S32750 and UNS S32760 respectively.

PREN

Pitting Resistance Equivalent Number = %Cr + 3.3x%Mo + 16x%N. A screening index for pitting resistance.

PREN-W

The tungsten-inclusive variant: %Cr + 3.3x(%Mo + 0.5x%W) + 16x%N. It credits F55's tungsten and narrows the gap between the two grades.

Critical pitting temperature (CPT)

The temperature at which pitting begins in ASTM G48-C ferric chloride testing. Higher is better.

Critical crevice temperature (CCT)

The equivalent measure for crevice corrosion under ASTM G48-D.

Ferrite window

The acceptable 30-60% ferrite fraction in duplex steel; outside it, toughness and corrosion resistance drop.

Sigma / chi phase

Brittle intermetallic phases that can form in duplex steel above roughly 250-300 degC, limiting the service ceiling.

NACE MR0175 / ISO 15156

The standard that qualifies metals for sour (H2S) oil-and-gas service, with hardness and temperature limits.

ASTM A923

Test method for detecting detrimental intermetallic phases in duplex stainless steels.

Comparing S32750 and S32760 for a project? Send your specification to JN Alloy for a grade recommendation and a quotation including material, testing and certification.

For extreme operating conditions, choose JINIE; for high-end manufacturing, rely on JINIE.
A one-stop solution for:
Difficulties in material selection, processing, inspection, and after-sales support.
Tel: +86 19339900211
Add: Shuangchuang Building, High-tech Industrial Development Zone, Lu'an City, Anhui Province, China
Copyright © ANHUI JINIE SPECIAL ALLOY CO.,LTD. All Rights Reserved.